Water-Soluble Temporary Solder Mask for High-Frequency PCB: Process and Reliability

Table of Contents

Solder mask ink is a kind of heat-resistant coating material. Workers coat it on designated regions of circuit boards.

It blocks solder paste adhesion in selected zones during soldering. This barrier prevents bridging short circuits and solder wastage.

Figure 1 illustrates the conventional solder mask workflow. Manufacturers finish electroplating of surface-mount circuit traces first.

Then they apply solder mask through a sequence of operations. Key steps include surface pretreatment, coating and curing.

Green ink dominates the PCB industry. It takes up over 90 percent of all solder mask products.

For this reason, people also call solder mask “green ink”.

Figure 1 Traditional PCB solder mask method
Figure 1 Traditional PCB solder mask method

Problem Description

Many high-frequency circuit products face strict coating limits.

Typical examples include microwave circuits, antennas and power electronic devices.

Their operating frequency usually falls within 2–4 GHz.

Designers cannot apply conventional green solder mask on these PCBs.

Electrical performance, structural requirements and reliability set this restriction.

The solder mask disturbs impedance matching. It also introduces substantial signal loss.

Additionally, antenna printed circuit boards come in single-layer and multilayer configurations.

In multilayer boards, we usually place feed solder joints on intermediate layers, so we cannot easily apply traditional green solder mask to the recesses in these layers.

Due to the lack of innovative solder mask solutions, the production of microwave circuits, antennas, and power electronics has traditionally relied on manual high-temperature tape application or no solder mask at all.

This poses significant challenges for product assembly, leading to issues such as insufficient solder, solder overflow, and short circuits at the solder joints, which adversely affect high-frequency transmission performance.

Specifically:

1) Insufficient Solder.

As shown in Figure 2, the absence of solder mask protection at the pad boundaries causes the solder to spread toward the periphery, preventing the formation of a proper solder joint at the connection point.

Figure 2 Poor soldering
Figure 2 Poor soldering
2) Solder Overflow.

As shown in Figure 3, in the absence of solder mask, the solder spreads to the surrounding interfaces, altering the material at the peripheral bonding or eutectic interfaces, which has a significant impact on back-end reliability.

Figure 3 Uncontrolled solder spread
Figure 3 Uncontrolled solder spread
3) Short Circuits.

Without a solder mask to prevent it, solder bridges form between two adjacent pads, causing a short circuit.

4) High High-frequency Transmission Losses.

We typically produce solder joints without solder mask protection by manual soldering.

This method delivers low efficiency and makes it hard to control solder volume, so the solder joints show poor consistency.

Excessive solder can impair transmission performance, leading to high losses during high-frequency transmission.

Furthermore, inconsistent solder joints significantly impact products requiring amplitude-phase consistency and increase debugging complexity.

The amount of solder can cause variations in the dimensions of the solder joints (both radially and axially).

We performed simulations using HFSS software to analyze how radial dimensional variations affect transmission performance.

A typical cascaded solder joint model revealed that changes in the radial dimensions of the solder joints have a significant impact on transmission performance.

Prototype Fabrication

Currently, 98% of printed circuit boards use photoresist solder mask, which is thermally or UV-cured to enhance its hardness, heat resistance, and chemical resistance.

In this study, we used water- or ethanol-soluble temporary solder mask materials.

We applied the temporary solder mask via printing or spraying before we soldered the circuit board.

After we finished circuit assembly and soldering, we removed the temporary solder mask with a water-based cleaning machine or solvent cleaning.

The process flow is shown in Figure 4.

Figure 4 Temporary solder resist path
Figure 4 Temporary solder resist path
  • Process Principle of Temporary Water-Soluble Solder Mask

We selected typical microwave substrates and components as the subjects of this study.

The test specimens and substrate design are shown in Figure 5.

Conventional thin-film resistors measuring 1 mm × 0.5 mm × 0.254 mm were used as components, with all six surfaces at both ends of the device featuring a gold-plated finish.

During assembly, we require soldered surfaces to form strong solder joints, while we prevent solder from wetting the top surface.

We designed the PCB pads for assembly according to surface-mount component pad design requirements.

These pads include two independent 0.6 mm × 0.6 mm pads with a center-to-center distance of 0.4 mm.

To better verify the solder joint integrity, we arranged the test specimens in a daisy-chain configuration.

Figure 5 Sample condition
Figure 5 Sample condition
  • Design of Test Specimens and Daisy-Chain Layout

Figure 6 presents simulation results of droplet evolution. Researchers run these calculations in Surface Evolver. Simulations cover droplet states a and b.

Total energy declines when liquid transforms from state a into state b. This downward trend in the energy curve supports the theory.

It lays a foundation for water-soluble solder mask approaches.

Figure 6 Droplet energy simulation
Figure 6 Droplet energy simulation
  • Surface Evolver Simulation of Solder Mask Droplet Evolution

Therefore, Chemask CW8 (whose main component is polyvinyl acetate), a water-soluble solder mask, was used to apply a solder mask to the upper surface of the thin-film resistor.

The requirement was that the solder mask cover more than 95% of the upper surface of the thin-film resistor; due to surface tension, the liquid solder mask did not flow onto the sides of the thin-film resistor.

Figure 7 shows the appearance of the film resistor after application of the water-soluble solder mask.

As we can see, the solder mask covers the upper surface of the film resistor and provides effective protection.

Furthermore, no solder mask has overflowed onto the sides of the film resistor, so it will not affect subsequent soldering.

The applied solder mask is then cured under the following conditions: 30 minutes at room temperature, or 15 minutes in an 80 °C oven for accelerated curing.

Figure 7 Resistance of water soluble solder resist after soldering
Figure 7 Resistance of water soluble solder resist after soldering

Validation Results

  • Solder Mask Removal

We conducted a design of experiments (DOE) together with the product assembly cleaning process to remove the water-soluble solder mask.

The Taguchi method was used to design process test parameters, combining common cleaning methods with different durations.

The detailed test parameters are as follows:

A: Soaking in anhydrous ethanol helps reduce the adhesion of the solder mask to the film resistor and loosens its material structure; we selected this factor for optimization at three levels.

B: Soaking time in modified Freon 141B.

We also use modified Freon, a common cleaning solvent, to reduce the adhesion between the solder mask and film resistor and loosen its material structure; we selected this factor for optimization at three levels.

C: Automated cleaning method. We typically subject PCBA assemblies to automated cleaning to remove contamination residues from the printed circuit board.

Under current conditions, we generally adopt three cleaning methods: spray, jet, and ultrasonic.

We selected this factor for optimization as a three-level factor.

The optimized experimental design is shown in Table 1, with three replicates per test sample.

No.Alcohol ConcentrationOxygen Flow RateAutomatic Cleaning
100Spray Cleaning
2015Spray Cleaning
3030Ultrasonic Cleaning
4150Spray Cleaning
51515Ultrasonic Cleaning
61530Spray Cleaning
7300Ultrasonic Cleaning
83015Spray Cleaning
93030Spray Cleaning

Table 1. L9 Orthogonal Experimental Design

1. Taguchi DOE Setup for Solder Mask Removal

Determining the main effect parameters for the Taguchi method evaluation:

P1: Residual area of water-soluble solder mask.

According to beam-type wire bonding requirements, the contaminated area on the film’s bonding surface must not exceed 40 percent.

The smaller the residual area of the water-soluble solder mask, the less impact it has on downstream bonding operations; therefore, this effect is a “minimize” attribute (see Table 2).

The residual conditions after cleaning are shown in Table 3.

No.Evaluation ItemAttributeValue
P1Area of Residual Adhesive on the SurfaceSmaller Is Better0

Table 2. Evaluation of the Field Test

Table 3 Results after cleaning tests
Table 3. Results after cleaning tests

We used software to calculate and analyze the area of solder mask residue.

The analysis results are listed in Table 3, while Figure 8 presents the main effect of the signal-to-noise ratio.

No.P1 – Sample 1P1 – Sample 2P1 – Sample 3
197.45%100%100%
216.8%45.27%37.43%
333%31.66%27.28%
461.15%59.46%67.62%
537.31%6.22%21.68%
60.58%2.06%1.32%
768.07%41.13%60.95%
816.70%47.08%34.78%
90%0%0%

Table 3. Residual Area Statistics

Figure 8 Main effect diagram of factors
Figure 8. Main effect diagram of factors

2. Signal-to-Noise Ratio Analysis and Optimal Parameter Combination

The recommended combination of cleaning processes is A2, B3, and C1; specifically, the process recommends cleaning with a spray washer following a Freon soak.

As shown in Figure 9, after a 15-minute soak in deionized water, the water-soluble solder mask underwent a significant color change—from blue to white—and its adhesion decreased substantially.

It could be easily removed by conventional brushing, which also achieved the desired removal effect.

Figure 9 Removal effect of deionized water
Figure 9 Removal effect of deionized water
  • Reliability

We generally characterize the reliability of resistors by solder joint strength and impedance, and thermal shock affects these components easily.

This research adopts thermal shock for accelerated life evaluation. Two tests assess the quality of resistor solder joints.

They include thrust testing and impedance measurement. Dye staining tests and interface characterization supply extra evidence.

Combined observations confirm the final microstructure state.

Tests follow the specification of standard QJ 3086A-2016. Operators place specimens inside a forced-air circulation oven.

Samples cycle between −55 °C and 100 °C. The cooling or heating rate to room temperature stays below 10 °C/min.

At each extreme temperature, the specimens were held for 15 minutes. The average duration of each cycle should be 1 h.

After 200 thermal cycles, the samples were inspected at a minimum magnification of 15×.

As shown in Figures 10 and 11, the P-value for the normality test of resistance data before and after thermal shock was less than 0.005.

A comparison of the resistance changes in the film before and after thermal shock revealed a variation of 0.8%, meeting the standard requirement that the resistance change be less than 20%.

We show the appearance of the solder joints after thermal cycling in Figure 12; we observe no microcracks.

As shown in Figure 13, we perform a staining test on the samples after thermal shock.

After staining, we separate the chip mechanically from the printed circuit board and examine the fracture surfaces of the circuit board and components under a microscope.

We find no crack failure at the solder joints after red ink staining. This result indicates that the solder joints can withstand 200 thermal shock cycles.

Figure 10 Normal distribution of resistance data
Figure 10 Normal distribution of resistance data
Figure 11 Resistance change before and after temperature punching
Figure 11 Resistance change before and after temperature punching
Figure 12 No cracking observed in the resistor after temperature punching
Figure 12 No cracking observed in the resistor after temperature punching
Figure 13 Red ink staining result after temperature breaking
Figure 13 Red ink staining result after temperature breaking

1. Thermal Shock and Dye Staining Reliability Tests

The results of the solder joint thrust test are shown in Table 4.

After we finished the thrust test, we analyzed the fracture surface under a microscope to identify the fracture mode.

No.Conductive Adhesive BondingResistance Before AgingResistance After Aging0402 Resistor
146013202461.82430
248013002305.42300
34507102465.92390
462015402023.02320
557014702511.72410
64005902240.32350
750014602172.32460
85715902259.32460
958014602426.72459
1051614101346.02402
1160110201329.92324
1242815502308.52368
1343114902233.82418
145969502199.12322
1540614201910.72354
1642115102122.22455
174759712029.72339
1861415032172.22414
1949310542182.92302
2047414262197.42383
216057842182.72308
225777231458.42415
2362010571633.42416

Table 4. Thrust Test Results(Unit: cN)

We performed statistical inference on the population based on the sample and acquired the following results:

At a 95% confidence interval, the film resistance before solder mask optimization was (1041.5 cN, 1319.0 cN), and after optimization, it was (1939.5 cN, 2226.0 cN).

We find that the film resist delivers much higher resistance strength after optimization.

Its thrust values approach those of widely used thick-film resistors, so it satisfies practical usage requirements.

2. Thrust Strength Test and Confidence Interval Analysis

As shown in Figures 1–4, the interface structure at the solder joints after assembly of the thin-film resistor, from the device body to the solder profile, is as follows: body → Au → Ni → Ni₃Sn₄ → SnPb.

The typical fracture morphology after thrust failure is shown in Figure 15.

Figure 15 Typical thrust port morphology
Figure 15 Typical thrust port morphology

We find from statistical analysis that thin-film resistors fracture mainly at the internal Au layer of the solder joints after thrust loading fails them.

This indicates that, in terms of the structural strength of the thin-film resistor solder joint interface, the strength at the IMC and solder locations exceeds that of the thin-film resistor plating structure, and the assembled solder joints are reliable.

Metallographic analysis also reveals that the morphology and thickness of the solder joint interfaces are consistent, and the bonding at the interfaces of the components is sound, as shown in Figure 16.

Figure 16 Metallographic results
Figure 16 Metallographic results

Conclusion

This paper introduces a solder mask technology for high-frequency circuit boards and draws the following conclusions:

1) Water-soluble solder mask effectively protects surfaces that do not require soldering and offers good workability.

2) Water-soluble solder mask can be removed by soaking in Freon followed by cleaning in a spray washer; it can also be effectively removed by soaking in deionized water.

3) The resistance to solder thrust has significantly improved following solder mask optimization.

4) Based on resistance testing and push force tests following thermal shock, combined with dye penetration testing and metallographic analysis, the soldering reliability of thin-film resistors using water-soluble solder mask meets the requirements.